Vibration During Welding At Power Plant (Steam Turbine)
PT. Semen Tonasa – Sulawesi Selatan

ABSTRACT WELDABILITY OF MATERIALS : TITANIUM AND TITANIUM ALLOYS * High strength to weight ratio
* Corrosion resistance
* Mechanical properties at elevated temperatures. KEYWORDS : Weld Metal Porosity, Embrittlement, Contamination Cracking, Vibration During Welding, Condensate, Tie Rod, Repair Welding, Conductivity. Introductions MATERIAL TYPES ALLOY GROUPINGS



FILLER ALLOYS * Titanium and its alloys can be welded using a matching filler. Composition; Compositions are given in
* The American Welding Society Specification AWS A5.16-2004.

WELD IMPERFECTIONS

WELD METAL POROSITY

EMBRITTLEMENT

CONTENT

CASE STUDY / WELDING REPAIR Power Plant at BTG Semen Tonasa - Pangkep Sulawesi Selatan is a coal steam turbine.
The condensate made from SS 410 with titanium lining (On tube sheet).
Join on Tube Sheet and Tie Rod is crack and sea water come inside to the boiler.
Problem..! So… we did repair welding on join tube sheet and tie rod.

 

CONTAMINATION CRACKING

 

FILLER TITANIUM

Titanium 6Al-4V AWS Class ER Ti-5

Features

Applications

 

 

 

Performance Profile

Ti 6Al-4V is the most widely used of all the alpha beta titanium alloys. Itmay be heat treated for high strength in welded construction at service temperatures through 600oF. Harden ability is limited and section over about one inch may not develop full properties. For cryogenic applications the extra low interstitial grade ELI (UNS R 56401) is preferred.

Annealing bar and forging is done at 1275-1325 oF 2hr air cool. Solution treat 1675-1725 oF 1hr water quench. Precipitation treat 975-1025 oF 3hr air cool. For increased fracture toughness but low tensile strength precipitation treat 1150 oF 4hr air cool.

Welding is by GTAW, direct current electrode negative, ¾ “ gas cup and gas lens. Limit electrode extension to 3/8 “. Inert gas shielding is required on all areas hotter than 800 oF. That is in addition to remarry torch shielding, trailing shield is required to protect the cooling weld metal, and back up shielding is required. Internal spaces should be purged 10 times the enclosed volume. Shield all tack welds.

Shielding and purge gas must be argon or argon helium mixture, NEVER nitrogen. Filler metal AWS A5.16 ERTi-5 may be used. ERTi-5 ELI preferred for greater toughness.

 

 

1.Sheet : Regular anneal furnace coolDuplex anneal. Mill anneal + 1435 oF, 15 minutes air cool. Triplex anneal. Mill anneal + 1850 oF, 5 minutes air cool, + 1375, 15 minutes air cool.

Bar and forgings :

Duplex anneal 1650-1850, 1 hour air cool + 1000oF -1100 oF, 8-24 hours air cool.

2.Bar duplex anneal : Mill anneal + 1000o – 1200oF, ½-6 hours air cool.

3.Anneal furnace cool at 300oF per hour maximum to 1000 oF to 1050 oF.

4.Stress relief may be accomplished at 800oF-15 hours, 850oF-5 hours, at 900oF-1 hour and 950 oF - ½ hour.

5.For 100% stress relief, 1000 oF -50 hours or 1200 oF -5 hours for 50% relief, 1000 oF -5 hours or 1100 oF – ½ hour.

6.Furnace cool at 300oF maximum from anneal temperature for maximum improved by holding at annealing temperature 24 hours.

 

7.Slow cool to 1000 o -1050 oF maximum from upper annealing temperature.

8.Anneal sheet at temperature for 20 minutes. For bar hold at anneal temperature 2 hours.

 

 .

 

Tie Rod Titanium 6 Al 4 V

 

Tie rod titanium condensate is support at tube sheet with loaded sea water = 250m3/minute.

 

 

 

Prepare before welding (Turbine off)

PENETRANT TEST (P.T)

After welding and cooling down, color on HAZ is looked silver (shielding gas maximum) Penetrant Test : accepted (No crack or porosity)

 

FUNGTIONAL TEST

Turbine on, water conductivity at condensate and hot well 70. When broken! Water conductivity 900. (Sea water conductivity 64,000).

Recommended for boiler <10, during operation before crack on join tube sheet & tie rod=8, After first repair conductivity 70…. Not accepted. After 2x24 hours… conductivity up to 4,000 and than shut down the turbine…!!

 

 

SECOND PREPAIRE (Turbine … Start Up)

1.Re-cleaned up on tube sheet & tie rod.

2.Re-make V groove on tube sheet & tie rod.

3.Re-welding process:

 

 

VACUUM TEST

84 Bar vacuum test with water soap… No broken (accepted)

PENETRANT TEST

On HAZ color… SILVER.

Penetrant test… No Crack or porosity.

FUNGTIONAL TEST

After 2x24 hours… Turbine running, conductivity=2.4…very good

Electric power connect to transmission.

 

Root pass… RPM 1000 ( Start up)

Filling …… RPM 2000 ( Start up)

Capping …. RPM 3000 (Running)

CONCLUSION :

Clean , clean and clean …is very important

Shield, shield and shield …is very important

Vibration During Welding is a way to the good welding of Titanium

REFERENCES


SUKARDI

www.arcmartindonesia.com